Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of PENTAMID AB L5 H1 RC black - PA66/6 - Pentac Polymer GmbH

Material Data Center offers the following functions for PENTAMID AB L5 H1 RC black:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Pentamid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Molding shrinkage, parallel 1.4 / * % ISO 294-4, 2577
Molding shrinkage, normal 1.4 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 2700 / 1200 MPa ISO 527
Yield stress 65 / 40 MPa ISO 527
Yield strain 4.5 / 17 % ISO 527
Flexural modulus, 23°C 2550 / - MPa ISO 178
Flexural strength 95 / - MPa ISO 178
Charpy impact strength, +23°C N / N kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 16 / 22 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 255 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 60 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 180 / * °C ISO 75-1/-2
Burning behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm -
Electrical propertiesdry / condUnitTest Standard
ISO Data
Relative permittivity, 1MHz 3.2 / - - IEC 62631-2-1
Electric strength 32 / - kV/mm IEC 60243-1
Comparative tracking index 525 / - - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 8.1 / * % Sim. to ISO 62
Humidity absorption 2.5 / * % Sim. to ISO 62
Density 1110 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
ISO Data
Viscosity number 130 / * cm³/g ISO 307, 1157, 1628
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 3 h -
Processing humidity ≤0.13 % -
Mold temperature 60 - 100 °C -
Feed temperature 80 °C -
Zone 1 265 °C -
Zone 2 275 °C -
Zone 3 280 °C -
Zone 4 285 °C -
Zone 5 280 °C -
Characteristics
Processing
Injection Molding
Delivery form
Pellets, Black
Special Characteristics
High impact or impact modified, Heat stabilized or stable to heat
Chemical Resistance
Oil Resistance
Certifications
Recycled Resin Content, RoHS compliant
Regional Availability
Europe
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com